为了提高直缝埋弧焊管多丝埋弧焊接速度,采用预热四丝埋弧焊接工艺进行了X60 钢级Φ559 mm×32 mm规格钢管焊接对比试验,并与常规四丝埋弧焊工艺进行对比.对比试验发现,与常规四丝埋弧焊工艺相比,采用预热四丝埋弧焊工艺时,可提高焊接速度 20%,降低焊接线能量 10%,整体力学性能优.证明预热多丝埋弧焊工艺在保证焊缝质量、力学性能的前提下,可以显著提高直缝埋弧焊管的焊接速度,是一种优质、高效、节能的埋弧焊新工艺.
Experimental Research on Pre-heating Multi-wire SAW Process for X60 Φ559 mm×32 mm LSAW Pipe
In order to increase the multi-wire SAW welding speed for the LSAW pipe,the welding comparative ex-periment for the X60 Φ559 mm×32 mm steel pipe is conducted via the pre-heating 4-wire SAW process,and a compa-rison with the conventional 4-wire SAW process is made.The result shows that compared with the said conventional 4-wire SAW process,the pre-heating 4-wire SAW process brings about such advantages as the welding speed is increased by 20%,the welding wire energy consumption is reduced by 10%,and the overall mechanical performance is excellent.It is proved that under the pre-conditions that the weld quality and the mechanical properties of the pipe are guaranteed,the above mentioned pre-heating multi-wire SAW process can obviously increase the welding speed for the LSAW pipe.

LSAW pipemulti-wire SAW processwelding wire pre-heatinghi-speed welding

赵波、赵与越、王能干、王强、安晓军、郭振其

展开 >

中国石油集团渤海石油装备制造有限公司,河北 青县 062658

中国石油天然气第六建设有限公司,广西 桂林 541004

直缝焊管 多丝埋弧焊 预热焊丝 高速焊

2024

钢管
攀钢集团成都钢铁有限责任公司

钢管

影响因子:0.755
ISSN:1001-2311
年,卷(期):2024.53(4)
  • 9