针对高磷铁矿因铁矿物与磷矿物共生关系复杂、常规选矿方法难以高效利用的特点,提出了焙烧—浸出的提铁降磷技术.对阿尔及利亚TFe品位为 60.81%、FeO含量为 14.92%、P含量为 0.71%的某高磷铁矿,采用悬浮焙烧(氧化焙烧—磁化焙烧)—磁选—浸出工艺开展了提铁脱磷实验研究,在氧化温度 1 050℃、还原温度 520℃、还原时间 25 min、H2 体积浓度 50%的磁化焙烧工艺条件下,获得了TFe品位 65.50%、TFe回收率 96.31%、P含量 0.16%的铁精矿指标,磷脱除率 77.46%.实验研究结果可为高磷铁矿提铁降磷提供指导.
Dephosphorization of a High-phosphorus Iron Ore by Magnetic Roasting-leaching Process
In response to the characteristics of high-phosphorus iron ore,which the complex symbiotic relationship between iron minerals and phosphate minerals in high-phosphorus iron ore and the difficulty in efficient utilization through conventional beneficiation methods.The roasting-leaching technology for iron extraction and phosphorus reduction was proposed with a view to achieving efficient utilization of high-phosphorus iron ore.This paper investigated a high-phosphorus certain iron ore with a TFe grade 60.81%,FeO content14.92%,and P content 0.71%extracted from Algeria.The experimental study on iron extraction and dephosphorization was carried out by oxidizing roasting-magnetization roasting-magnetic separation-leaching process.The magnetic roasting process conditions of oxidation temperature 1 050 ℃,reduction temperature 520 ℃,reduction time 25 min and H2 concentration 50%were determined.The iron concentrate indexes of total Fe grade 65.50%,total Fe recovery 96.31%and P content 0.16%were obtained,which 77.46%of P removed.The experimental results offer guidance for iron extraction and dephosphorization of iron ore in Algeria.

high-phosphorus iron oreoxidizing roastingmagnetic roastingleaching

王绍兴、宁国栋、刘应志、李艳军

展开 >

上海逢石科技有限公司,上海 201600

东北大学 资源与土木工程学院,辽宁 沈阳 110819

难采选铁矿资源高效开发利用技术国家地方联合工程研究中心,辽宁 沈阳 110819

高磷铁矿 氧化焙烧 磁化焙烧 浸出

2024

矿产保护与利用
中国地质科学院郑州矿产综合利用研究所

矿产保护与利用

CSTPCD
影响因子:0.592
ISSN:1001-0076
年,卷(期):2024.44(1)
  • 18