Abstract
Incomplete NH_3 decomposition is a major challenge in direct-NH_3 solid oxide fuel cells (DA-SOFCs) which limits cell performance. Herein, we propose to employ thermally stable NH_3 decomposition catalysts in DA-SOFCs during NH_3 fueling. The Ba/Ni/Al_2O_3 catalyst synthesized from a layered double hydroxide via rapid hybrid microwave annealing shows high Ni dispersion and suppresses particle migration. The Ba/Ni/Al_2O_3 achieved 82 % NH_3 conversion at 550 ℃ with an H_2 production rate of 26.8 mmol g_(cat)~(-1) min~(-1). Furthermore, the catalyst-integrated DA-SOFC achieved a peak power density of 0.56 W cm~(-2) at 650 ℃ under NH_3, comparable to that under H_2-N_2 conditions (0.61 W cm~(-2)). In contrast, a commercial DA-SOFC fed with NH_3 exhibited a significantly lower peak power density of 0.43 W cm~(-2). These results demonstrate that integrating an active catalyst with DA-SOFCs enables efficient on-site H_2 generation and utilization in NH_3-fueled power systems.